UNCLASSIFIED

28.
29.

Now carry out a final 75% HNOg sevaration in the 250 ml

beaker. (100 ml volume)

Filter through a fluorothene funnel cn a glass fibre filter.
Transfer the funnel to a clean filter flask and wash out the
acid with anhydrous ethyl ether.

Place the filter on a brass disc and ring assembly (Tracerlab),
cover with 0.001 inch plicfilm and § count.

Recovery values are of the order of 75% for the procedure as shown.

This method was selected initially to be certain of obtaining the
strontium regardless of its state. However, tests of leaching
methods showed good recoveries, and they are to be preferred for
handling large samples of soil. The following data gives a comparison of results by different methods.

Sample No.

Source

1

112

Albany, H.Y.

11,

Logan, Utah

98

Lamont Labs.

Method (a/m/g)

0.1420.08

2

3

0.1120.007

0.0920.006

© 0.1670.05 0.01220.002

-0870 .04

-08=0 04

-

-

Meth gods

1.

Complete solution as described.

2.

Leaching 10 minutes with 6 N HCl.

3.

Leaching 10 minutes with 1 N Ammonium Acetate.

The properties and abundance of the long-lived fission products were
given in the section on bone analysis. The effect of addition of the
following mixture of possible interferences in the enslysis of 100
gram soil wamples is given in Table A-=7.

kath CO
UNCLASSIFIED